WhatsApp

Article

The cold-end line that decides HRSG uptime: staying above the acid dew point

beta-pramesti-asiaindustry-power-generation-combinedprocess-ccgt

The cold-end line that decides HRSG uptime: staying above the acid dew point

In heat-recovery steam generators (HRSGs), a few degrees can separate high efficiency from tube leaks. The fix is to keep the coldest economizer surfaces hotter than the acid dew point of the flue gas, and to pick materials that survive the slips.

Industry: Power_Generation_(Combined_Cycle_Gas_Turbine_ | Process: _CCGT)

Cold-end corrosion is the quiet saboteur inside many HRSGs (heat recovery steam generators). Sulfuric or hydrochloric acids form from SO₂/NO₂/O₂ reactions with moisture. When they condense on steel surfaces that are too cool, they eat through economizer tubes and force outages. The acid dew point for typical flue gas is usually 100–150 °C, depending on fuel sulfur/chlorine and moisture content (digitalrefining.com).

The failure mechanism is plain in field reports. “The metal had fallen below the acid dew point, and therefore H₂SO₄ had condensed on the outer surface of the economizer tubes, causing severe corrosion,” one boiler-service analysis concluded (researchgate.net). Another plant burning high-sulfur oil traced economizer leaks to “acid dew point corrosion” from fuel sulfur (researchgate.net).

The chemistry is unforgiving. When any tube wall drops below dew point, condensing acids rapidly strip protective oxides, pit the metal, and thin the wall. Corrosion rates peak roughly 15–20 °C below the dew point. Letting flue gas fall just 20–30 °C below dew point can “max out” acid deposition and corrosion rate (vganapathy.tripod.com, tetra-eng.com).

Acid dew point, defined and quantified

Acid dew point is the temperature at which acid vapors (such as H₂SO₄ or HCl) in flue gas condense into liquid on cooler surfaces. It varies with fuel sulfur/chlorine content and moisture. For HRSGs with ~15% H₂O in the exhaust, it is usually 100–150 °C (digitalrefining.com). Kewanee guidance lists dew points of ~150 °C for natural gas and up to 180–200 °C for oil fuels (scribd.com). If economizer tube walls dip below those temperatures, sulfuric acid condenses and attacks the steel (researchgate.net, tetra-eng.com).

Natural gas can be benign, but not always. Even with low sulfur, plants still apply a margin. Conservative practice keeps the coldest economizer surfaces at least about 10–20 °C above the highest expected acid dew point (vganapathy.tripod.com).

Setpoint strategy: feedwater above dew point

Design and operational rule: keep the coldest economizer tube above the acid dew point of the flue gas, so the acids stay in the vapor phase. In practice, plants raise the feedwater or deaerator temperature, or add high‑pressure feedwater preheaters, so the economizer inlet water is hot enough. Kewanee’s classic table implies economizer feedwater of about 210 °C or more to cover dew points up to about 200 °C. Operators keep the economizer exit (feedwater inlet) 10–60 °C above dew point (scribd.com).

Rules of thumb back this up. Raise economizer feedwater at least ~10–15 °C above the acid dew point. Ganapathy’s note shows that lowering economizer feed by 40 °F (≈22 °C) usually improves cycle efficiency by ~1%, but only if acid corrosion is addressed (vganapathy.tripod.com, vganapathy.tripod.com). Raising flue gas temperature has little impact on economizer wall temperature. The wall temperature closely follows the water temperature (vganapathy.tripod.com).

For context (implied by the same Kewanee data), "safe" temperatures look like this. Natural gas has a dew point of ~40–100 °C with feedwater ≳60–110 °C (depends on specifics). #2 fuel oil (∼0.3–0.5% S) has a dew point of ~150–180 °C with feedwater ≳210 °C. Low‑Sigit fuel oil (∼2% S) has a dew point of ~180–200 °C with feedwater ≳220 °C (scribd.com).

Startup, shutdown, and layup controls

Shutdowns are a prime risk. At one site, upper economizer tubes cooled to ~80 °C during layup. They later failed from acid dew point corrosion (powermag.com). Plants counter this with recirculation of warm water or purging with dry gas. At the Terry Bundy combined‑cycle plant, dedicated recirculation pumps run during layup "to mitigate acid dew point corrosion" on HP/LP circuits (power-eng.com).

Chemistry helps too. Some operators switch to a protected layup chemistry, [oxygen scavengers and corrosion inhibitors](https://beta.co.id/en/blog/inside-the-hrsg-feedwater-playbook-scavenge-oxygen-raise-ph-cut-corrosion), to passivate surfaces. In practice, this can mean starting an oxygen scavenger program in the layup circuit. Also, a targeted corrosion inhibitor can reduce corrosion rates by 90%+ (product specification). South Humber Bank (UK) used a VpCI fog to protect economizer tubes (~80 °C during shutdown) after repeated dew‑point corrosion failures (powermag.com). Another option is full drying and nitrogen or dry‑air blanketing. These methods prevent condensation, but they can fail if seals leak.

Design details matter. Insulation should remove cold spots. Routing and baffles should avoid drafts and give even heat transfer. Online dew point sensors, frequent SO₂/SO₃ analyses and even stack condensate pH give early warning. Therefore operators can raise feedwater or adjust firing before condensation starts.

Economizer materials and corrosion resistance

Materials are the second line of defense. Carbon steel (for example ASME SA178 GrA/P1) is common and cost‑effective, but it has almost no resistance to condensing acids. Designs assume only a small corrosion allowance (≈1/32″) and expect no condensation (esteemprojects.com).

Stainless steels raise the bar. Austenitics like SS304L and SS316L resist acid attack. 316L has 2–3% Mo, so it is preferred for H₂SO₄. Tests show 316L has minimal attack versus carbon steel in sulfuric acid (researchgate.net). A 316L or 317L economizer can essentially eliminate dew point corrosion. Several units with high‑S or high‑chloride risks retrofit these tubes. The trade‑offs are 3–5× the material cost of carbon steel, sometimes lower thermal conductivity, and weld considerations.

Duplex/ferritic stainless steels give moderate H₂SO₄ resistance (better than 304, less than 316). However, they are not enough when condensation forms below ~150 °C. 5–9%Cr steels (P91, etc.) have little resistance to sulfuric or hydrochloric acids. [Nickel alloys—Inconel 625/825, Incoloy 800/825](https://beta.co.id/en/blog/inside-nickels-acid-gauntlet-how-hpal-plants-pick-metals-that-survive) resist H₂SO₄ and HCl much better (Incoloy 825 can withstand concentrated sulfuric acid). However, their cost limits them to the important sections. Clad options (carbon steel base with SS or Ni alloy cladding) isolate the substrate. 304‑clad economizers are used. Thermally sprayed and epoxy coatings usually do not last in continuous HRSG service.

Other materials, including polymers/composites, have been proposed for below‑dew‑point heat recovery. Thermoplastics like PPS‑GRP were tested. However, these remain experimental and not mainstream for utility HRSGs (digitalrefining.com, bcinsight.crugroup.com). In practice, the choice is an economic trade‑off. One economizer tube failure can cost tens of thousands in repairs plus megawatts in lost output. Upgrading all economizer tubing to 316L might raise material cost by only a few percent of a new HRSG budget, and it can reduce failures to near‑zero. Many units on sulfur‑bearing fuels specify stainless or NEWS (Ni alloy) cladding in sensitive sections. Some CCGTs in petrochemical service use 316L or even Incoloy bundles.

Note: even with good materials, acid exposure can still occur during wet layup or if chlorine drives HCl condensation at ~30–50 °C.

Efficiency targets versus corrosion margins

Operators usually look for lower flue gas temperatures to get better efficiency. If the flue gas outlet temperature drops by about 40 °F (≈22 °C), cycle efficiency usually improves by about 1% (vganapathy.tripod.com). However, when the gas comes close to the acid dew point and crosses it, corrosion gets worse. Conservative practice keeps a cushion of 10–20 °C above the dew point for the coldest tubes. Industry analysis also notes that recovering an extra 2–3% of flue heat by approaching the dew point can give several MW of extra output on a large unit (digitalrefining.com). This shows the tension between heat rate and reliability.

Monitoring and diagnostics

Plants track the economizer outlet temperature and the flue gas composition to make sure the coldest tube wall never goes below the dew point. You can monitor the remaining risk through the SO₂/SO₃ concentration and the stack condensate pH. If the dew point comes close to the planned tube temperature, operators raise the feedwater temperature or adjust the firing to stay clear of condensation (tetra-eng.com).

Indonesia’s fuel and policy context

Indonesia's combined-cycle fleet mostly burns natural gas or distillate. Both are very low in sulfur. Emission policy reinforces this. The Ministry of Environment and Forestry's MOEF Reg. 15/2019 pushes toward low-sulfur fuels or scrubbers. For coal units, flue gas desulfurization (FGD) usually washes SO₂ to <5% of inlet. One Indonesian coal project asked for ~95% SO₂ removal (irt.co.id). Indonesia caps SO₂ at 750 mg/Nm³ for ≥100 MW units (cybertig.com). Modern LNG and diesel are at <0.5% S. Therefore typical acid dew points may only be ~50–100 °C. Even so, you need dew-point margins and careful layups. Globally, HRSG tube failures remain common. Flow-accelerated corrosion and acid dew-point corrosion together usually account for >50% of tube damage cases.

The practical playbook

The guidance is consistent across studies. Keep economizer feedwater above the acid dew point of the flue gas, and design for the coldest tube to maintain the margin (vganapathy.tripod.com, scribd.com). Combine this with disciplined layup practices, targeted chemistry, and, where justified, corrosion‑resistant tubing. That combination preserves availability and heat rate. It keeps acids in the vapor phase and away from steel.

Sources for mechanism, setpoints, and cases: researchgate.net, tetra-eng.com, vganapathy.tripod.com. Layup and chemistry practices and site examples: powermag.com. Shutdown circulation: power-eng.com. Materials and allowances: esteemprojects.com. Policy and efficiency context: irt.co.id, cybertig.com, digitalrefining.com.